THERMAL
CONDUCTIVITY & R VALUE
|
|
DOKUZ
EYLUL UNIVERSTY, IZMIR / TURKEY ENGINEERING FACULTY
DEPARTMENT OF MECHANICAL
ENGINEERING
|
|
REPORT
|
Subject:
Evaluation of Thermal Conductivity Coefficient
Company: DBS
Insaat Taah Kimya San ve Tic Ltd Sti
|
| |
|
Material received by our department
(Wall Mix G and Wall Mix W) were tested with the QTM machine, utilizing
the hot wire method. Resulting average thermal conductivity values are
given below:
|
| |
|
Sample
Name
|
Testing
Environment
Temperature (°C)
|
Thermal
Conductivity
Coefficient (W/mK)
|
|
Wall Mix
G
|
25
|
0,661
|
|
Wall Mix
W
|
25
|
0,787
|
- Thermal resistance (R value) =
L/k, measured in K·m2·W-1
|
| |
|
According the average thermal
conductivity values of Wall Mix G and Wall Mix W, thermal resistance
values may calculate with different thicknesses like given examples
below:
| R Values K·m2·W-1
|
Wall
Mix G
|
Wall
Mix W
|
| 0,5 cm thickness of application
|
0,008 m2K/W
|
0,006 m2K/W
|
| 1,0 cm thickness of application
|
0,015 m2K/W
|
0,013 m2K/W
|
| 2,0 cm thickness of application
|
0,030 m2K/W
|
0,025 m2K/W
|
| 2,5 cm thickness of application
|
0,038 m2K/W
|
0,032 m2K/W
|
|
|
THERMAL
CONDUCTIVITY- TEST REPORT (TURKISH)
|
|
|
|
|